A. Damage or defects that have gone through to the metal surface

Rusting or deformation:

(1) Feather edge the damaged area.
(2) Prepare the metal surface.
(3) Apply a chemical coating to the metal surface. Metal conditioner, Precoat, A.C.P treatment.
(4) Apply an undercoat (primer surfacer).
(5) Apply an intermediate coat (color matched to top enamel paint).
(6) Apply a top coat (body color paint).

Solid color: Enamel top coat paint
Metallic color: Metallic enamel paint + Clear top coat
Pearl color: Pearl enamel paint + Clear top coat

B. Damage or defects up to undercoat or intermediate coat.

For external damage or blisters, perform through under Item A.
For external damage only perform under Item A.

C. Damage or defects that have not gone through to intermediate coats (only in top coat)

Shallow scratches or score marks:
1. If damage has gone through to the metallic paint, spray metallic enamel, then apply top coat wet on wet.
2. If damage has not reached the metallic color paint and remained in the clear top coat,polish the damaged surface or spray only the clear top

coat.

NOTE:  Try to repair by polishing as much as possible if the damage has not reached the metallic color paint.

D. Replacement of Parts Welded parts

Rear side outer panel, etc.
1. Perform step (1) through (6) if the damaged area is covered with filler or welded with reinforcement plate.
2. Perform steps (5) and (6) for undercoats except those on joints (Intermediate coat for replacement parts).
3. On inner panels, apply paint where the undercoat is burned by welding heat. Follow this with a rust preventive treatment.

Single Parts
-

Painting the outer and inner hood, door, trunk, lid, etc. Perform steps under Item A.

-

Painting the inside of the front fender.
Only enamel top coat paint may be used on solid color enamel, metallic enamel, or pearl enamel.

-

After spraying enamel paint, perform rust preventive treatment (apply inner or outer rust preventive agent).

Refinishing Procedures

Refinishing Procedures

1. Featheredging (polishing damaged areas).

Damage to metal surface

-

Sand the damaged area flat and smooth with a double action sander and #60 or 180 disc paper.

-

Sand the boundary between the metal surface and undercoat with a double action sander and #180 or #280 disc paper. Try to sand a larger area
than the damage.

NOTE:
-

Make sure there is no height difference between the metal surface and undercoat,

-

If double action sander is not available. use a rubber block and wrap sandpaper around it to sand the surface.

WARNING:  To prevent eye injury, wear goggles or safety glasses whenever sanding, cutting, or grinding.

Damage to Undercoat

Intermediate coat
Top coat
Paint coat on replacement parts

Sand the damaged surface flat and smooth with a double action sander and #280 or #320 paper.

NOTE:  
-

If double action sander is not available, use a rubber pad and wet or dry sand the surface with #280, #320, #400, or #600 sandpaper.

-

After sanding, check that the surface is flat and smooth.

-

Perform the operations provided in "damage to metal surface" above for the areas where parts are welded to the body.