Super ponacle II, Solo de Diamont, Diamont (R-M)

-

Autocryl Auto base (Akzo)

-

Super Centari (DuPont)

Primer/Primer surfacer:
Use when the resin material is exposed.

-

R-M fast filler + R-M flex primer (R-M)

-

Plasto flex primer 2 coat (Akzo)

-

1220RH-S filler primer (DuPont)

Repair Procedures

Repair Procedures

A. Deep scratches, when filling:

1. Sand the damage section. (#120-#240)
2. Apply the filler and dry.
3. Sand the filler (#240-#400)
4. Coat with the primer/primer surfacer and dry.
5. Sand the primer surfacer. (#600-#800)
6. Top coating.

B. Shallow scratches:

1. Coat with the primer/primer surfacer.
2. Sand the primer surfacer. (#600-#800)
3. Top coating.

C. Repaint:

1. Sand the primer surfacer. (#600-#800)
2. Top coating.

Refinishing Procedures

Refinishing Procedures

1. Base material reconditioning (sanding)

1. Repaint the replacement part

Lightly sand the part with #400, #600 or #800.

2. Slight scores or scratches

Use a flexible sanding block, wet sand the damaged section with #400, #600 sandpaper.

NOTE:  Sand level to remove damage.

3. Deep scratches when filling.

Use a flexible sanding block and wet sand the damaged section with #240 #400 sandpaper.

2. Degreasing and cleaning

Clean the repaired area with wax and grease remover, then blow with compressed air

WARNING:
-

Do not use high air pressure; use only an approved, 210 kPa (2.1 kgf/sq.cm, 30 psi) air nozzle.

-

Wear goggles or safety glasses to prevent eye injury.