Plastic Bumper - Refinishing Techniques|Page 5601 > < Plastic Bumper - Refinishing Techniques|Page 5599
Page 4
background image

2.

Clearcoat Chroma Base Basecoat with Chroma Clear High Glamour 7800S or Chroma Clear MULTI Use 7500S.

6b.

NON BasecoatiClearcoat Procedures

Topcoat with Chroma One Single Stage according to label direction.

BASF Glasurit Procedure

Bumper Cover Preparation PUR or PP

1.

Pre-baking the bumper cover at 140° F for 45 minutes will improve adhesion.

2.

Wash the bumper cover with soap and water.

3.

Dry with paper towel and lint-free cloth.

4.

Wash with Glasurit 541-30 Universal Plastic Cleaner to remove wax, silicone and contaminates. Dry with paper towel.

5.

Scuff the entire bumper cover with gray Scotchbrite pad.

6.

Wash off residue with 541-30.

7.

Allow to dry completely with lint-free cloth.

Coating PUR (Polyurethane) bumper covers

8.

Apply 1 thin uniform coat of Glassofix 934-0 1K Plastic Adhesion Primer.

9.

Allow 15 to 20 minute flash time.

10.

Apply Glasurit L-21 or L-54 to hiding. In the case of L-21, use 40 volume parts of Glassodur 521-111 Elastifier Additive according to procedure.

11.

In the case of L-54, allow 15 to 20 minutes flash time.

12.

Apply either Glassodur 923-54 or 923-85 with 20 volume parts Glassodur 521-111 Elastifier Additive according to label directions (or compliant
clear for VOC regulated areas).

Coating PP (Polypropylene) bumper covers

8.

Apply 1 thin uniform coat of Glassodur 285-0 2K Transparent Filler.

9.

Allow 15 to 20 minute flash time.

10.

Apply a thin coat of Glassodur 285-75 Tintable Primer if necessary.

11.

Apply Glasurit L-21 or L-54 to hiding. In the case of L-21, use 40 volume parts of Glassodur 521-111 Elastifier Additive according to procedure.

12.

In the case of L-54 allow 15 to 20 minutes flash time.

13.

Apply either Glassodur 923-54 or 923-85 with 20 volume parts Glassodur 521-111 Elastifier Additive according to label directions (or compliant
clear for VOC regulated areas).

Herberts Standox Procedures

Bumper Cover Preparation PP (polypropylene)

1.

Bake for 60 minutes at 140° F (60° C) to temper the plastic.

2.

Clean the product several times using a Gray Scotch Brite pad and Standoflex 11100 Thinner anti-static cleaner (use a clean pad and fresh thinner
with each cleaning.).

3.

Allow to dry completely.

4.

As a final clean before priming, use fresh Standoflex 11100 Thinner anti-static cleaner with a clean towel.

Bumper Cover Preparation PUR (polyurethane)

Plastic Bumper - Refinishing Techniques|Page 5601 > < Plastic Bumper - Refinishing Techniques|Page 5599