CL TYPE S V6-3.2L SOHC (2001)
-
Apply the putty on the damaged area in 2-3 steps.
-
Glue aluminum tape on the outside of the bumper, and apply putty from the other side of the bumper.
-
Remove the aluminum tape after the putty dries, apply putty from the outside, and fill the hole.
Use a special polyester putty (Reference) and a putty knife.
3. Sanding
Sand the surface evenly, particularly at the area where the PP material and putty meet.
Use a flexible block and #240-#400-#600 sand paper.
4. Air blowing / degreasing
Use alcohol, a tack cloth, and wax and grease remover.
5. Spraying primer surfacer
NOTE: Spray the bumper primer on the area where the PP material was exposed and around the putty.
-
Spray the primer surface wider than the putty and painted surfaces of bumper primer.
-
Spray 2 to 3 coats to get 20 to 30 microns of thickness.
-
Use the 2-component type primer surfacer (gray) and a spray gun.
-
Follow the materials manufacturer's instructions.
Drying
NOTE: Take care not to let the heat lamp deform the bumper during the drying process.
6. Sanding
After drying, wet sand the area of the intermediate coat.