Paint: Service and Repair
Soft Chipping Guard Primer Coat

General

The removal of paint and Undercoating by stone chips immediately exposes metal to the atmosphere, causing it to oxidize. The thickness of this
oxidation increases if the process continues unchecked. The soft chipping guard primer protects against damage due to the impact of such objects.

-

The soft chipping guard primer coat is applied over the E.D. (Electrostatically Deposited) primer. It is followed by guide coating and top coating.

-

The soft chipping guard primer produces a smooth surface when dry. It should be sprayed so the thickness of the protective film is 20 microns

Basic Rules for Repairing a Soft Chipping Guard Primer Coat:

-

Soft chipping guard primer coat is then applied to the most susceptible area.

-

Spray the primer surface (2-part urethane primer surfacer) on the soft chipping guard primer coating areas when you replaced parts using soft
chipping guard primer coat.

WARNING:
-

Wear goggles or safety glasses to prevent eye injury.

-

Ventilate when spraying undercoat.

1. Sanding the replacement part.

NOTE:
-

Do not oversand the edges or corners of the part.

-

Do not expose base metal.

Use a double action sander and #400 disc sandpaper.

2. Air blowing/degreasing

Use alcohol, and wax and grease remover.

3. Masking

Use masking tape and paper.

4. Spraying primer surfacer

-

Spray 4-5 coats to get 20 microns of thickness. One coat deposits 5-7 microns.

-

Do not try to cover the surface with one heavy coat. Apply several thin coats.