9-3 Arc/Aero (9440) L4-2.0L Turbo (2.0 T) (2004)
Spoiler: Procedures
Bumper and Spoiler, Deep Scratches and Cracks
Bumper And Spoiler, Deep Scratches And Cracks
1. Clean the component. It is important to insure that there is no gravel or other particles in the welding area.
2. Clean the area to be repaired with Teroson FL cleaner.
3. Identify the type of plastic. See Plastic codes, temperature and welding wire or Plastic code table.
4. Select the correct welding wire and set the welding gun to an operating temperature appropriate for the plastic type. See Plastic codes, temperature
and welding wire
5. If the damage is a crack, first drill at the ends so the crack does not spread. Use a 3.5 mm bit to drill a hole at each end of the crack.
6. Cut a 90 degrees V-joint on the back. Use a low-speed machine.
7. Set the welding gun to an operating temperature appropriate for the plastic type.