6b.

NON Basecoat/Clearcoat Procedures

Topcoat with Chroma One Single Stage according to label direction.

BASF Glasurit Procedure

Bumper Cover Preparation PUR or PP

1.

Pre-baking the bumper cover at l40°F for 45 minutes will improve adhesion.

2.

Wash the bumper cover with soap and water.

3.

Dry with paper towel and lint-free cloth.

4.

Wash with Glasurit 541-30 Universal Plastic Cleaner to remove wax, silicone and contaminates.

Dry with paper towel.

5.

Scuff the entire bumper cover with gray Scotchbrite pad.

6.

Wash off residue with 541-30.

7.

Allow to dry completely with lint-free cloth.

Coating PUR (Polyurethane) bumper covers

8.

Apply 1 thin uniform coat of Glassofix 934-01K Plastic Adhesion Primer.

9.

Allow 15 to 20 minute flash time.

10.

Apply Glasurit L-21 or L-54 to hiding. In the case of L-21, use 40 volume parts of Glassodur 521-111 Elastifier Additive according to procedure.

11.

In the case of L-54, allow 15 to 20 minutes flash time.

12.

Apply either Glassodur 923-54 or 923-85 with 20 volume parts Glassodur 521-111 Elastifier Additive according to label directions (or compliant
clear for VOC regulated areas).

Coating PP (Polypropylene) bumper covers

8.

Apply 1 thin uniform coat of Glassodur 285-02K Transparent Filler.

9.

Allow 15 to 20 minute flash time.

10.

Apply a thin coat of Glassodur 285-75 Tintable Primer if necessary.

11.

Apply Glasurit L-21 or L-54 to hiding. In the case of L-21, use 40 volume parts of Glassodur 521-111 Elastifier Additive according to procedure.

12.

In the case of L-54 allow 15 to 20 minutes flash time.

13.

Apply either Glassodur 923-54 or 923-85 with 20 volume parts Glassodur 521-111 Elastifier Additive according to label directions (or compliant
clear for VOC regulated areas).

Herberts Standox Procedures

Bumper Cover Preparation PP (polypropylene)

1.

Bake for 60 minutes at 140°F (60°C) to temper the plastic.

2.

Clean the product several times using a Gray Scotch Brite pad and Standoflex 11100 Thinner anti-static cleaner (use a clean pad and fresh thinner
with each cleaning.).

3.

Allow to dry completely.

4.

As a final clean before priming, use fresh Standoflex 11100 Thinner anti-static cleaner with a clean towel.

Bumper Cover Preparation PUR (polyurethane)

1.

Bake for 60 minutes at 140°F (60°C) to temper the plastic.